Sains Malaysiana 49(12)(2020): 3169-3177
http://dx.doi.org/10.17576/jsm-2020-4912-28
The Influence of
Temperature and Electroforesis Deposition Green
Inhibitor on Bipolar Plate AA5052 in Sulfuric Acid Medium
(Pengaruh Suhu dan Endapan Elektroforesis Perencat Hijau pada Plat Dwikutub AA5052 dalam Asid Sulfurik)
I GUSTI
AYU ARWATI1,3, EDY HERIANTO MAJLAN1*, LOH KEE SHYUAN1,
TEUKU HUSAINI1, SAGIR ALVA3, MUHAJIRIN3 &
NABILAH AFIQAH MOHD RADZUAN2
1Fuel
Cell Institute, Universiti Kebangsaan Malaysia, 43600 UKM Bangi, Selangor Darul Ehsan, Malaysia
2Centre
for Materials Engineering and Smart Manufacturing, Faculty of Engineering and
Built Environment, Universiti Kebangsaan Malaysia, 43600 UKM Bangi, Selangor Darul Ehsan, Malaysia
3Engineering
Faculty, Mercu Buana University, 11650 Jakarta Barat, Indonesia
Received:
4 August 2020/Accepted: 11 September 2020
ABSTRACT
Aluminum
alloy 5052 (AA5052) contains Mg (2.2-2.8.8% weight), Cu (0.1% weight), Cr
(0.15% weight), Zn (0.1% weight), Si and Fe (0.45% weight) compositions. This
material has been widely used as a bipolar plate in Proton exchange Membrane (PEMFC) fuel cells. This material has several advantages such as:
lightness, high conductivity, good tensile strength, and flexibility. PEMFC
operations produce several by-products, such as water and heat. Generally, the
operation of PEMFC is around 333-353 K and the environment is acidic. In this condition
the bipolar plate AA5052 will easily experience rust, thus lowering the
performance of the PEMFC. In this study, 0.5 g/L Arabic Gum (AG) used as a
green inhibitor and coated onto the AA5052 surface through electrophoretic
deposition (EPD). The corrosion test was performed in 0.5 M H2SO4 (pH 2) solution under the simulated PEMFC condition. Scanning electron
microscopy (SEM) was used to analyze the morphology, and potentiodynamic polarization to determine the corrosion rate. Result shows that AG coating can
reduce 60% the corrosion rate of AA5052 after immersed in 0.5 M H2SO4 for 168 h. The effect of temperature on the inhibition efficiency reached 14.4%
under the same condition. AG can be used as a green inhibitor to reduce the
corrosion rate of AA5052 bipolar plate.
Keywords:
Aluminum alloy 5052; Arabic Gum inhibitor; corrosion rate; electrophoretic
deposition
ABSTRAK
Aloi aluminium 5052 (AA5052) mengandungi komposisi Mg (2.2-2.8.8% berat),
Cu (0.1% berat), Cr (0.15% berat),
Zn (0.1% berat), Si dan Fe
(0.45% berat). Bahan ini telah digunakan secara meluas sebagai plat dwikutub untuk sel fuel membran pertukaran proton
(PEMFC). Bahan ini digunakan kerana kelebihannya, seperti ringan, kekonduksian tinggi, kekuatan tegangan yang baik dan kefleksibilannya. Operasi PEMFC menghasilkan beberapa produk sampingan seperti air dan haba. Secara amnya, PEMFC beroperasi pada suhu 333-353 K dan mempunyai persekitaran yang berasid. Plat dwikutub AA5052 ini akan mudah mengalami karat, sehingga menurunkan prestasi PEMFC. Dalam kajian ini, 0.5 g/L Gam Arab (GA) digunakan sebagai perencat hijau dan dilapisi ke permukaan AA5052 melalui pemendapan elektroforetik (EPD). Ujian kakisan dilakukan dalam larutan 0.5 M H2SO4 (pH 2) sesuai dengan simulasi keadaan PEMFC. Mikroskopi elektron imbasan (SEM) digunakan untuk menganalisis morfologi dan polarisasi potensiodinamik untuk menentukan kadar kakisan. Hasil menunjukkan bahawa lapisan AG dapat mengurangkan 60% kadar kakisan AA5052 setelah direndam dalam 0.5 M H2SO4 selama 168 jam. Kesan suhu pada kecekapan penghambatan mencapai 14.4% dalam keadaan yang sama. AG boleh digunakan sebagai perencat hijau untuk mengurangkan kadar kakisan AA5052.
Kata kunci: Aloi aluminium 5052; kadar kakisan; pemendapan elektroforesis; perencat Gam Arab
REFERENCES
Ameh, P.O. 2014. Inhibitory action of Albizia zygia gum on
mild steel corrosion in acid medium. African
Journal of Pure and Applied Chemistry 8(2): 37-46.
Arwati, I.A., Majlan,
E.H., Daud, W.R.W., Shyuan,
L.K., Arifin, K., Husaini,
T., Alva, S. & Radzuan, N.A.M. 2019.
Electrophoresis deposition Arabic Gum effect on aluminum 5052 reduce corrosion. Sains Malaysiana 48(2): 401-406.
Arwati, I.A., Majlan,
E.H., Daud, W.R.W. & Alva, S. 2018. Temperature
effects on stainless steel 316L corrosion in the environment of sulphuric acid (H2SO4). IOP Conference Series: Materials Science and
Engineering 343(012016): 1-8.
Azzaoui, K., Mejdoubi, E., Jodeh, S., Lamhamdi, A., Rodriguez-Castellón,
E., Algarra M., Zarrouk,
A., Errich, A., Salghi, R.
& Lgaz, H. 2017. Eco friendly green inhibitor Gum
Arabic (GA) for the corrosion control mild steel in hydrochloric acid medium. Corrosion Science 129: 70-81.
Besra, L. & Liu, M. 2007. A review
on fundamentals and applications of electrophoretic deposition (EPD). Progress in Materials Science 52(1):
1-61.
Bhowmik, A., Srivas, S.P. & Khandelwal,
A.K. 2016. A review of the properties aluminium alloy
5052. Journal of Scientific Research in
Allied Science 2(2) 25-30.
Boccacini, A.R., Keim, S., Ma, R., Li, Y. & Zhitomirsky,
I. 2010. Review: Electrophoretic deposition of biomaterials. Journal of the Royal Society Interface 7(5):
581-613.
Chiang,
T.Y., Su, A., Tsai, L.C., Sheu, H.H. & Lu, C.E.
2014. Corrosion resistance of 5052 Al-alloy with a Zirconia-rich conversion
coating used in bipolar plates in PEMFCs. International
Journal of Electrochemical Science 9: 5850-5863.
Choudhary, B., Anwar, S., Besra, L. & Anwar, S. 2017. Electrophoretic deposition
studies of Ba(Zr-Ce-Y)O3 ceramic coating. International Journal of
Applied Ceramic Technology 16(3): 1022-1031.
Dalo, M.A., Othman, A. & Al-Rawashdeh, N.A.F. 2012. Exudate gum from acacia trees as
green corrosion inhibitor for mild steel in acidic media. International Journal of Electrochemical Science 7: 9303-9324
Dariva, C.G. & Galio,
A.F. 2014. Corrosion inhibitors - principles, mechanisms and applications. In Developments in Corrosion Protection,
edited by Aliofkhazraei, M. Rijeka: InTech. pp. 365-379.
Denni Asara Awizar, Norinsan
Kamil Othman, Azman Jalar, I. Abdul Rahman & N.H. Al-hardan. 2013. Nanosilicate extraction from rice husk ash green corrosion
inhibitor. Journal of Elechtrochemical Science 8: 1759-1769.
Gharavi, F., Matori, K.A., Yunus, R., Othman,
N.K. & Fadaeifard, F. 2015. Corrosion behavior of
Al6061 alloy weldment produced by friction stir welding process. Journal of Materials Research and Technology 4(3): 314-322.
González
Gutiérrez, A.G., Sebastian, P.J., Magallón Cacho, L., Borja Arco, E., Campos, J. & Baron, A. 2018.
Surface modification of aluminum alloy 6061 for bipolar plate application:
Adhesion characteristics and corrosion resistance. International Journal of Electrochemical Science 13: 3958-3969.
Huang,
N.B., Yu, H., Xu, L.S., Zhan, S., Sun, M. & Kirk, D.W. 2016. Corrosion
kinetics of 316L stainless steel bipolar plate with chromium carbide coating in
simulated PEMFC cathodic environment. Results in Physics 6: 730-736.
Khan,
G., Kazi, S.N., Basirun,
W.J., Ali, H.B.M., Faraj, F.L. & Khan, G.M. 2015.
Application of natural product extracts as green corrosion inhibitors for
metals and alloys in acid pickling processes - a review. International Journal of Electrochemical Science 10: 6120-6134.
Pech-Rodríguez, W.J., González-Quijano, D., Vargas-Gutiérrez, G. & Rodríguez-Varela,
F.J. 2014. Electrophoretic deposition of polypyrrole/Vulcan
XC-72 corrosion protection coatings on SS-304 bipolar plates by asymmetric
alternating current for PEM fuel cells. International
Journal of Hydrogen Energy 39(29): 16740-16749.
Sagir Alva, Aiman Sajidah
binti Abdul Aziz, Mohd Ismahadi bin Syono & Wan Adil bin Wan Jamil. 2018.
Ag/AgCl reference electrode based on thin film of
Arabic Gum membrane. Indonesian Journal
of Chemistry 18(3): 479-485.
Sutharssan, T., Montalvao, D., Kang, Y., Wang, W., Pisac,
C. & Elemara, H. 2017. A review on prognostics
and health monitoring of proton exchange membrane fuel cell. Renewable and Sustainable Energy 75:
440-450.
Taherian, R. 2014. A
review of composite and metallic bipolar plates in proton exchange membrane
fuel cell: materials, fabrication, and material selection. Journal of Power Sources 265: 370-390.
Umoren, S.A. & Eduok,
U.M. 2016. Application of carbohydrate polymers as corrosion inhibitors for
metal substrates in different media: A review. Carbohydrate Polymer 140: 314-341.
Vadivelan, M.R., Kumar,
N.S. & Balaji, R. 2015. A review on corrosion of
metallic bi-polar plates for proton exchange membrane (PEM) fuel cells. IOSR Journal of Mathematics 11(6):
83-99.
Yang,
Y., Guo, L.J. & Liu, H. 2011. Corrosion
characteristics of SS316L as bipolar plate material in PEMFC cathode
environments with different acidities. International
Journal of Hydrogen Energy 36(2): 1654-1663.
Zhang,
D., Duan, L., Guo, L.,
Wang, Z., Zhao, J., Tuan, W.H. & Niihara, K.
2011. TiN-coated titanium as the bipolar plate for
PEMFC by multi-arc ion plating. International
Journal of Hydrogen Energy 36(15): 9155-9161.
*Corresponding author; email: